The oxygen index (limiting oxygen index, LOI) test measures the minimum oxygen concentration required to sustain candle-like combustion of polymeric materials, and its results are strongly influenced by test temperature and the humidity conditioning of specimens. This article compares the major oxygen index testing standards—ISO 4589-2 and ISO 4589-3, EN ISO 4589, ASTM D2863, GB/T 2406, and JIS K 7201—alongside the conditioning specifications in ISO 291 and ASTM D618 that define how temperature and humidity are controlled before and during testing.
Technical Overview
The oxygen index (OI), also known as the limiting oxygen index (LOI), is defined as the minimum concentration of oxygen, expressed as a volume percentage in a flowing oxygen/nitrogen mixture, that will just support candle-like combustion of a vertically mounted specimen. Under the principal ambient-temperature standards—ISO 4589-2, EN ISO 4589-2, ASTM D2863, GB/T 2406.2, and JIS K 7201-2—the specimen passes the test if it burns for less than 180 seconds or over a distance of less than 50 mm after top-face ignition. Because ambient air contains approximately 21% oxygen, materials with an LOI above 21% tend not to continue burning in still air at room temperature, and many industry specifications set minimum LOI values in the range of 26% to 32% for flame-retardant grades.
Temperature and humidity are not incidental variables in this test; they are controlled parameters with dedicated standards. ISO 4589-2 and its equivalents specify testing at a gas temperature of 23 ± 2 °C, while ISO 4589-3 and GB/T 2406.3 extend the method to elevated temperatures using a heated test column. Specimen conditioning prior to testing is governed by ISO 291, GB/T 2918, and ASTM D618, which define standard atmospheres such as 23 °C/50% relative humidity. As a general rule, the measured LOI decreases as test temperature rises, because thermal decomposition becomes easier, while absorbed moisture in hygroscopic polymers acts as a heat sink and diluent that can raise the apparent LOI. Understanding these effects, and the differences between the various standards, is essential when comparing data sheets or specifying tests at accredited third-party laboratories.
Testing Samples
Rigid and Semi-Rigid Plastic Mouldings
Under ISO 4589-2, EN ISO 4589-2, and GB/T 2406.2, the preferred rigid specimen is 80 to 150 mm long, 10 mm wide, and 4 mm or 10 mm thick, cut or moulded with smooth edges free of burrs and flash. ASTM D2863 uses a smaller standard specimen, typically 70 to 150 mm long, 6.5 ± 0.5 mm wide, and 3 ± 0.5 mm thick, which is one reason results from the two systems may not be directly interchangeable.
Films, Sheets, and Flexible Materials
Thin and flexible materials that cannot stand upright unsupported are tested using special preparation techniques, such as winding the film on a mandrel or supporting it in a frame, as permitted by the annexes of ISO 4589-2 and corresponding provisions in ASTM D2863. Flexible elastomeric sheets are also tested in this configuration.
Cellular Materials and Foams
Rigid and flexible foams are tested as rectangular strips using specimen holders designed to avoid compressing or distorting the cells. The standard atmosphere and conditioning requirements apply equally to foams, and their strongly temperature-dependent burning behaviour makes elevated-temperature testing particularly informative for these materials.
Textile Fabrics
Burning behaviour of textiles by the oxygen index method is covered in the Chinese national system by GB/T 5454, which specifies strip specimens cut in both warp and weft directions. This method is widely applied to flame-retardant fabrics used in public assembly venues, transport seating, and protective applications.
Testing Items
Accredited third-party laboratories typically offer the following oxygen index test items, which differ in the temperature of the test and the humidity conditioning applied beforehand:
- Ambient-temperature oxygen index at 23 ± 2 °C per ISO 4589-2, EN ISO 4589-2, ASTM D2863, GB/T 2406.2, or JIS K 7201-2
- Elevated-temperature oxygen index per ISO 4589-3 or GB/T 2406.3, commonly at specified temperatures between approximately 70 °C and 150 °C depending on the equipment capability
- Oxygen index after standard conditioning at 23 °C and 50% relative humidity for a minimum of 88 hours per ISO 291 or GB/T 2918
- Oxygen index after dry conditioning, for example over desiccant or in a ventilated oven, per ASTM D618 procedures or material specification
- Oxygen index after humid preconditioning at elevated humidity levels such as 40 °C/95% RH, 70 °C/95% RH, or 85 °C/85% RH where required by product or purchase specifications
- Temperature-dependence studies in which the LOI is determined at several temperatures to characterise how flame retardancy changes across the service temperature range
Testing Methods
Apparatus and Principle
All oxygen index methods use a vertical heat-resistant glass chimney, a specimen holder, a calibrated gas mixing and flow-control system supplying oxygen/nitrogen mixtures at a constant total flow rate, and a small diffusion flame igniter applied to the top of the specimen. The oxygen concentration is adjusted in a bracketing sequence until the critical concentration is found at which the pass/fail criterion of 50 mm burn length or 180 seconds burn time is just met. The result is reported as the oxygen index in volume percent, together with the specimen dimensions, orientation, conditioning history, and test temperature.
Ambient-Temperature Procedure
For ISO 4589-2, EN ISO 4589-2, ASTM D2863, GB/T 2406.2, and JIS K 7201-2, conditioned specimens are mounted vertically, the chimney is purged with the gas mixture, and the top edge is ignited. Concentration steps are narrowed progressively, and the LOI is calculated from the oxygen concentrations bracketing the transition between burning and self-extinguishing behaviour. The gas mixture is maintained at laboratory ambient temperature, nominally 23 ± 2 °C.
Elevated-Temperature Procedure
ISO 4589-3 and GB/T 2406.3 employ a test column fitted with electrical heating and thermostatic control so that both the gas mixture and the specimen reach the specified elevated temperature before ignition. Specimens are pre-heated at the set temperature for a defined soak period, after which the standard ignition and bracketing procedure is performed. Because flame-retardant mechanisms such as char formation and intumescence weaken at elevated temperature, the LOI measured under ISO 4589-3 is generally lower than the room-temperature value and provides a more realistic assessment for components operating in hot environments.
Temperature and Humidity Conditioning
ISO 291 and its Chinese counterpart GB/T 2918 define the standard conditioning atmospheres of 23 °C/50% RH (with 27 °C/65% RH recognized for tropical climates) and specify a minimum conditioning period of 88 hours for most plastics. ASTM D618 Procedure A specifies 40 hours at 23 ± 2 °C and 50 ± 5% RH, with alternative procedures for dry conditioning. Where a product specification requires worst-case assessment, laboratories can precondition specimens at high temperature and humidity, or after oven drying or water immersion, before carrying out the oxygen index determination. The conditioning state must always be reported, since moisture content can shift the LOI of hygroscopic materials such as polyamides and cellulose-based polymers by a measurable margin.
Key Differences Among the Standards
- Specimen geometry differs: ISO 4589-2 and GB/T 2406.2 use 10 mm wide, 4 to 10 mm thick specimens, whereas ASTM D2863 uses 6.5 mm wide, 3 mm thick specimens
- Temperature scope differs: ISO 4589-2, ASTM D2863, GB/T 2406.2, and JIS K 7201-2 cover ambient temperature, while ISO 4589-3 and GB/T 2406.3 cover elevated temperature
- Conditioning references differ: the ISO and GB systems reference ISO 291/GB/T 2918, while ASTM D2863 references ASTM D618
- Adoption status differs: EN ISO 4589-2 and JIS K 7201-2 are directly aligned with ISO 4589-2, while GB/T 2406.2 is a modified adoption, so minor procedural differences may exist
- Because of these differences, LOI values obtained under different standards should not be compared without confirming that specimen size, conditioning, and test temperature were equivalent
Applications
Oxygen index testing under controlled temperature and humidity conditions supports a wide range of engineering and compliance activities:
- Research and development screening of flame-retardant formulations in plastics, rubber, and composite materials
- Quality control of flame-retardant compounds used for cable insulation and sheathing, complementing the vertical flame tests of the IEC 60332 series and the small-scale burning tests of UL 94
- Material qualification for rail vehicle and public transport interiors, where materials must demonstrate fire performance across the operating temperature range
- Marine and shipbuilding applications, where naval engineering specifications have historically set demanding minimum LOI values for onboard materials
- Aerospace interior components, storage systems, and engineering plastics requiring high LOI at both room and elevated temperatures
- Flame-retardant textiles for hotels, auditoriums, and mass transport seating, verified through GB/T 5454 or equivalent textile oxygen index methods
- Support of regulatory submissions and supplier declarations, with test reports issued by accredited third-party laboratories under ISO/IEC 17025 quality systems
FAQ
Why do temperature and humidity affect oxygen index results?
Raising the test temperature supplies additional energy that accelerates pyrolysis and generally lowers the oxygen concentration needed for sustained burning. Humidity acts in the opposite direction for hygroscopic materials: absorbed water absorbs heat and dilutes combustible decomposition products, which can raise the measured LOI. This is precisely why the standards mandate defined conditioning atmospheres and, in the case of ISO 4589-3, defined elevated test temperatures.
What is the difference between ISO 4589-2 and ISO 4589-3?
ISO 4589-2 determines the oxygen index at ambient temperature, nominally 23 °C, in a standard chimney without heating. ISO 4589-3 uses a heated test column and pre-heated specimens to determine the oxygen index at a specified elevated temperature, giving an indication of flame retardancy under hot service conditions.
Are ASTM D2863 and ISO 4589-2 results interchangeable?
Not automatically. Although the principle is identical, the two standards prescribe different specimen dimensions, conditioning references, and certain procedural details. For critical comparisons, the same standard, specimen geometry, conditioning history, and test temperature should be used.
What oxygen index value counts as flame retardant?
A material with an LOI above approximately 21% will typically not continue burning in still air at room temperature. In practice, industry specifications commonly require LOI values of 26% to 32% or higher for flame-retardant grades, and some transport and marine applications additionally require verification at elevated temperature.
Which conditioning atmosphere should be applied before testing?
Unless a material or product specification states otherwise, ISO 291 and GB/T 2918 conditioning at 23 °C and 50% relative humidity for at least 88 hours applies to ISO and GB system tests, while ASTM D618 Procedure A (40 hours at 23 °C and 50% RH) applies to ASTM D2863. Special applications may specify dry, humid, or immersed preconditioning to simulate worst-case service exposure.
Can laboratories perform oxygen index tests at custom temperature or humidity conditions?
Yes. Accredited third-party laboratories equipped with heated oxygen index apparatus can test at selected elevated temperatures per ISO 4589-3 or GB/T 2406.3, and can apply bespoke humidity or drying preconditioning before a standard ISO 4589-2 or ASTM D2863 determination, provided the deviations from the standard conditions are clearly documented in the test report.
Why Choose ZKGX?
- State-of-the-art analytical equipment
- Highly qualified scientific team
- Fast turnaround time
- Competitive pricing