The experimental procedure for preparing deposited metal chemical analysis specimens ensures that weld metal chemistry is measured on representative, undiluted material deposited under controlled welding conditions. Aligned with ISO 6847, ISO 15792-1, GB/T 25774.1, and AWS A5.01, this guide explains test pad deposition, sampling, machining, cleaning, and the analytical techniques used to verify welding consumable composition. It serves as a practical reference for welding engineers, metallurgical laboratories, and quality professionals involved in consumable qualification and certification.
Technical Overview
Deposited metal is the filler metal that has been melted, transferred through the arc, and solidified to form the weld. Because it constitutes the actual material of the finished joint, its chemical composition is the primary basis for the classification, certification, and acceptance of welding consumables such as covered electrodes, solid wires, metal-cored and flux-cored wires, submerged arc wire and flux combinations, and gas tungsten arc filler rods. The experimental procedure for preparing deposited metal chemical analysis specimens defines how a representative test pad is deposited and how a specimen is extracted, machined, cleaned, and preserved so that the reported composition reflects the consumable itself rather than dilution, slag entrapment, or handling contamination.
Every preparation code is built on the same three principles: eliminate dilution by the base plate, exclude slag, oxide, and foreign matter, and deliver the specimen in a physical condition suited to the intended analytical technique. The principal governing references include:
- ISO 6847 — Welding consumables, deposition of a test weld and preparation of a test specimen for chemical analysis
- ISO 15792-1 — Welding consumables, test methods, all-weld metal test specimens
- GB/T 25774.1 — Chinese national standard for all-weld metal test specimen preparation, technically aligned with ISO 15792-1
- AWS A5.01/A5.01M and the AWS A5.xx filler metal specifications — weld pad requirements for chemical analysis
- ISO 14284 and the GB/T 223 series — sampling and chemical analysis of steel and iron
- ASTM E415, ASTM E1019, ASTM E572, JIS G 1253, and GB/T 4336 — instrumental determination methods for metallic matrices
Testing Samples
Covered Electrode Deposits (SMAW)
A multi-layer weld pad is deposited on a clean base plate whose composition does not interfere with the elements to be determined; low-carbon steel plate is typical for carbon and low-alloy ferritic consumables. The pad is built in successive layers, commonly a minimum of three to four depending on electrode diameter, and the specimen is taken only from the undiluted region lying a specified minimum height above the fusion line, generally 3 mm to 5 mm as required by the applicable specification. This guarantees that the measured composition represents pure deposited metal rather than a mixture with the base plate.
Wire, Rod, and Flux-Cored Deposits (GMAW, FCAW, GTAW, SAW)
Machine-welded pads permit tight control of heat input, travel speed, and shielding, producing highly uniform material. For submerged arc combinations, the flux chemistry actively participates in metallurgical reactions, so the specific wire and flux pairing, including flux baking and reclaim limitations, must be documented and reproduced. Gas-shielded processes require verified gas composition and flow rates, since shielding quality affects oxygen and nitrogen pickup and, indirectly, retained alloy content.
Specimen Forms Submitted for Analysis
- Drillings or millings (chips) — required for combustion infrared analysis, ICP-OES, atomic absorption, and classical wet chemistry
- Flat-ground solid coupons — required for spark discharge optical emission spectrometry (OES) and X-ray fluorescence screening
- Crushed solid pieces or buttons — used for inert gas fusion determination of oxygen and nitrogen
Typical minimum quantities are approximately 20 g to 50 g of chips for a full elemental suite, plus a solid coupon of suitable area for OES, with surplus material retained as an archived sample for verification testing.
Testing Items
The elemental scope depends on the consumable classification being verified. Common testing programs include:
- Base elements for carbon steel consumables: C, Si, Mn, P, S
- Low-alloy additions: Cr, Ni, Mo, V, Nb, Ti, B, Cu, Al
- Stainless steel and duplex grades: Cr, Ni, Mo, N, Cu, with control of ferrite-stabilizing and austenite-stabilizing balances
- Hardfacing and special alloys: W, Co, Mn, high Cr, and carbide-forming elements
- Residual or tramp elements (As, Sn, Sb, Pb) restricted in pressure vessel, nuclear, and low-temperature applications
- Gas content (O, N) where specified for cleanliness-sensitive or high-strength classifications
Testing Methods
Test Pad Deposition
The base plate is prepared by grinding and degreasing, positioned flat, and welded in the PA position unless the specification directs otherwise. Run-on and run-off sections or tabs absorb arc initiation and extinction irregularities and are discarded before sampling. Welding parameters are held within the consumable manufacturer's recommended range, and interpass temperature is monitored and controlled, commonly below 250 °C for carbon steel classifications and as stipulated by the classification standard for creep-resisting and low-alloy grades. Complete traceability records linking the specimen to the consumable heat number, lot, diameter, and deposition parameters are maintained.
Sampling and Machining
After cooling, the slag is fully removed and the oxidized top layer is machined away to expose sound, clean weld metal. Chips are then produced by slow-speed drilling or milling using clean, sharp carbide or hardened tool steel cutters, machining dry or with clean compressed air to avoid coolant contamination. Excessive feed speed is avoided because frictional heating can oxidize or discolor chips and locally alter surface composition. Chips are collected on clean, lint-free surfaces, never by hand, and magnetic separation is applied to capture any metallic tool debris.
Cleaning and Preservation
The specimen is degreased in acetone or ethanol, air-dried, and sealed in moisture-proof, labeled containers identifying the consumable, heat number, specimen form, and preparation date. Chips intended for oxygen or nitrogen determination, or for reactive elements, are stored in a desiccator and analyzed promptly to prevent surface oxidation from biasing results.
Analytical Techniques and Method Alignment
- Combustion infrared absorption for carbon and sulfur — ASTM E1019, ISO 15350, and the GB/T 223 series provide the benchmark for low-level accuracy
- Spark discharge optical emission spectrometry for routine multi-element analysis — ASTM E415, GB/T 4336, GB/T 11170, and JIS G 1253
- ICP-OES and atomic absorption spectrometry for trace and minor alloying elements such as Ti, B, Nb, and V
- X-ray fluorescence screening of solid coupons — ASTM E572 and equivalent national methods
- Inert gas fusion for oxygen and nitrogen — ASTM E1019 and corresponding national standards
Quality assurance requires the use of certified reference materials matrix-matched to weld metal, duplicate determinations, and documented measurement uncertainty, particularly when results are reported for certification by accredited third-party laboratories.
Applications
- Classification and certification of welding consumables against AWS A5.1, A5.5, A5.17, A5.18, A5.20, A5.28, and A5.29, as well as EN ISO 2560, 14341, and 17632
- Conformity assessment of consumables under structural welding codes and construction products regulations
- Approval programs administered by classification societies and other certification bodies for marine, offshore, and pressure equipment applications
- Supporting data for welding procedure qualification records where all-weld metal composition is required
- Incoming inspection, lot verification, and screening of suspect or counterfeit consumables
- Research and development of new formulations, correlating composition with hardness, creep strength, and corrosion performance
- Failure analysis in which the actual delivered weld metal chemistry must be established as a baseline for investigation
FAQ
Why must the analysis zone sit at a minimum height above the base plate?
The first weld layers mix with melted base plate material, so their composition is diluted and unrepresentative. Sampling at or above the specified minimum height, combined with removal of the initial layers, guarantees the specimen is composed exclusively of undiluted deposited metal from the consumable under test.
Can a production weld be used instead of a dedicated test pad?
Generally no. Classification testing requires a dedicated pad deposited under the controlled conditions of ISO 6847 or the applicable AWS A5.xx specification. Some welding procedure qualification standards permit analysis of a production-type test piece, but only with explicit restrictions, and such results cannot substitute for consumable classification.
What is the minimum specimen mass required?
Approximately 20 g of chips typically suffices for carbon, sulfur, and major alloying elements, while a full multi-technique program with replicate determinations may require 50 g or more. Spark OES additionally requires a solid, flat-ground coupon large enough to seal against the spark stand, and surplus material is always retained for verification.
Why is overheating during chip machining prohibited?
Frictional heating causes surface oxidation and can drive pickup of carbon or alloying elements from cutting tools, biasing results for exactly the elements being measured. Slow, dry machining with sharp carbide tooling and clean collection practice preserves specimen integrity.
Which technique is most reliable for carbon and sulfur?
Combustion infrared absorption, performed per ASTM E1019, ISO 15350, or the GB/T 223 series, is the reference approach, especially at low concentration levels. Spark OES is acceptable for routine screening when calibrated and verified with appropriate reference materials.
How long can prepared chips be stored before analysis?
Sealed, dry chips stored in a desiccator remain stable for weeks for most elements, but specimens destined for oxygen, nitrogen, or highly reactive element determination should be analyzed as soon as practicable after preparation to limit surface oxidation effects.
Why Choose ZKGX?
- State-of-the-art analytical equipment
- Highly qualified scientific team
- Fast turnaround time
- Competitive pricing